Monprene IN-22958D XRD1 is a high performance thermoplastic elastomer designed specifically for demanding industrial applications including slip coats. Monprene IN-22958D is a high hardness, low density, UV stabilized, unfilled grade with a low coefficient of friction that can be processed by extrusion, co-extrusion and thin extrusion coating.
General Information
Features
  • Low Specific Gravity
  • Without Fillers
  • Low density
  • High smoothness
  • Light stabilization
  • Good UV resistance
  • Good adhesion
  • Medium liquidity
  • Lubrication
  • High hardness
Uses
  • Thin coating
  • Washer
  • Industrial application
  • Pipe fittings
  • Rubber substitution
  • Profile
RoHS Compliance
  • RoHS compliance
Appearance
  • Natural color
Forms
  • Particle
Processing Method
  • Co-extrusion molding
  • Extrusion
  • Coating
PhysicalNominal ValueUnitTest Method
Specific Gravity 0.888g/cm³ASTM D792
Melt Mass-Flow Rate (MFR) (230°C/2.16 kg)10g/10 minASTM D1238
HardnessNominal ValueUnitTest Method
Durometer Hardness ASTM D2240
    Shaw D, 1 sec 56ASTM D2240
    Shaw D, 5 seconds 53ASTM D2240
ElastomersNominal ValueUnitTest Method
Tensile Stress 1ASTM D412
    Transverse flow : 100% strain 10.2MPaASTM D412
    Flow : 100% strain 12.8MPaASTM D412
    Transverse flow : 300% strain 10.7MPaASTM D412
    Flow : 300% strain 13.1MPaASTM D412
Tensile Strength 2ASTM D412
    Transverse flow : Fracture 12.2MPaASTM D412
    Flow : Fracture 14.8MPaASTM D412
Tensile Elongation 3ASTM D412
    Transverse flow : Fracture 350%ASTM D412
    Flow : Fracture 660%ASTM D412
Tear Strength 4ASTM D624
    Transverse flow 81.3kN/mASTM D624
    Flow 153kN/mASTM D624
Compression Set 5ASTM D395B
    23°C, 22 hr 26%ASTM D395B
    70°C, 22 hr 57%ASTM D395B
Legal statement
The information and recommendations contained in this bulletin are, to the best of our knowledge, accurate and reliable but no guarantee of their accuracy is made. All products are sold upon condition that purchasers shall make their own tests to determine the suitability of such products for their particular purposes and uses and purchaser assumes all risks and liability for the results of use of the products, including use in accordance with seller's recommendations. Nothing in this bulletin constitutes permission or a recommendation to practice or use any invention covered by any patent owned by this company or others. There is no warranty of merchantability and there are no other warranties for the products described. For detailed Product Stewardship information, please contact us. Any product of Teknor Apex, including product names, shall not be used or tested in medical or food contact applications without the prior written acknowledgement of Teknor Apex as to the intended use. Please note that some products may not be available in one or more countries.
ExtrusionNominal ValueUnit
Cylinder Zone 1 Temp. 204 - 227°C
Cylinder Zone 2 Temp. 204 - 227°C
Cylinder Zone 3 Temp. 204 - 227°C
Cylinder Zone 4 Temp. 204 - 227°C
Cylinder Zone 5 Temp. 204 - 227°C
Die Temperature 204 - 227°C
Extrusion instructions
Screw Speed: 30 to 100 rpm;Drying is not necessary. However, if moisture is a problem, dry the pellets for 2 to 4 hours at 150°F (65°C).
Note Message
1 .C mold, 510mm/min
2 .C mold, 510mm/min
3 .C mold, 510mm/min
4 .C mold, 510mm/min
5 .Type 1
Resin Grade Manufacturer Category Trademark
Tecnoflon® FOR 9383 Solvay Specialty Polymers Fluorelastomer Tecnoflon®
TECHNYL® C 216 V15 BLACK 61 Solvay Engineering Plastics Nylon 6 TECHNYL® C
Texin® 985 Covestro - PUR TPU-Polyether Texin®
Plantic® R1 Plantic Technologies Limited Biodeg Polymers Plantic®
Plaslube® PA6/6,6 109 L Techmer Engineered Solutions Nylon 66/6 Plaslube®